GMAW on Aluminum Flashcards

You may prefer our related Brainscape-certified flashcards:
1
Q

Up to what length of contact tip is best suited for GMAW with aluminum filler wires?

a) 25.4mm
b) 50.8mm
c) 76.2mm
d) 101.6mm

A

d) 101.6mm

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
2
Q

List 3 advantages of using GMAW on aluminum

A

a) high deposition rates compared to GTAW
b) can be used long distances from the power source
c) no flux or slag, no inclusions in the weld material
d) clean up time is reduced or eliminated
e) may be used in all positions
f) works well on materials 3.2mm and up
g) works well for spot welding operations

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
3
Q

which aluminum filler metal is not recommended for sustained high temperature service?

a) 2319
b) 4145
c) 4043
d) 5356

A

d)5356

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
4
Q

What 3 factors should you consider when setting GMAW welding parameters

A

a) material thickness
b) alloy type
c) available equipment

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
5
Q

What effect does stickout have on arc length with GMAW on aluminum

A

the electrical stickout is not as critical as that required for steel. very little change in arc length is noticed with various stickout distances.

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
6
Q

After pre-cleaning aluminum, you should weld the joint:

a) with copper backing bar to prevent oxide contamination.
b) before it dries to prevent cracking
c) after age hardening has occured
d) as soon as all liquids have evaporated from the joint area

A

d) as soon as all liquids have evaporated from the joint area

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
7
Q

what precaution but you take when using heavy wire brushing or an abrasive grinding to remove a heavy oxide layer from aluminum?>

A

heavy brushing or abrasive discs tend to drive the aluminum oxides into the metal surface and entrap them. The result is possible contamination of the weld.

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
8
Q

what are the two most commonly used filler metals for GMAW on aluminum

a) 2319 and 4145
b) 4145 and 5356
c) 4043 and 4047
d) 4043 and 5356

A

d) 4043 and 5356

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
9
Q

What is the purpose of a light preheat on aluminum alloys?

a) to remove moisture
b) to reduce residual stresses after welding
c) easier arc starting
d) to remove surface oxides

A

a) to remove moisture

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
10
Q

What type of current do you use with GMAW for welding aluminum?

a) AC
b) DCEP
c) DCEN
d) AC with continuous high frequency

A

b) DCEP

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
11
Q

What methods can you use to fill a crater?

A

reverse trave direction for a short distance. run-off tabs, breaking and restarting the arc,

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
12
Q

What electrode inclination is recommended for the welding of aluminum

A

forehand at all times

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
13
Q

Most shielding gases for GMAW on aluminum are:

a) inert gases
b) oxidizing gases
c) nitriding gases
d) ionized gases

A

a) inert gases

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
14
Q

The shielding gas most commonly used with GMAW on non-ferrous metals is:

a) carbon dioxide
b) nitrogen
c) helium
d) argon

A

d) argon

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
15
Q

list 4 causes of burn back

A

a) wire feed speed too slow
b) worn or dirty contact tube
c) worn or dirt liner
d) wrong polarity
e) kinked electrode wire
f) liner too ling
g) arcing inside the contact tube

How well did you know this?
1
Not at all
2
3
4
5
Perfectly
16
Q

what happens when you use a backhand inclination when using GMAW on aluminum?

a) lack of fusion
b) the wire tends to burn back into the contact tube
c) a black soot oxide appears on the surface
d) excessive bead convexity

A

c) a black soot oxide appears on the surface

17
Q

Preheat applied t oaluminum components is:

a) done using inductance heating methods only
b) seldom required to exceed 149 C
c) not applied unless the ambient temperature is below -18
d) done only prior t isolation heat treating

A

b) seldom required to exceed 149 C

18
Q

The recommended technique and metal transfer for GMAW on aluminum is:

a) a pulsed spray transfer with a long stickout
b) forehand (pushing) inclination with short circuit or spray transfer
c) backhand (pulling) inclination with spray transfer
d) fast travel speed with continuous high frequency current transfer

A

b) forehand (pushing) inclination with short circuit or spray transfer

19
Q

What element causes porosity in an aluminum weld?

a) oxygen
b) nitrogen
c) carbon dioxide
d) hydrogen

A

d) hydrogen

20
Q

What can happen if you leave a crater at the end of an aluminum weld?

a) cracking
b) porosity
c) slag inclusions
d) hard spots

A

a) cracking